100CRMO7-4

4 source records. Standards, editions and conditions are presented separately; matching grade names do not establish interchangeability.

Refer to each source for mass fractions and analysis type. Missing values are not treated as 0. Manufacturer typical values, standard guarantees and measured heat results must remain separate. Use the material selector for calculations and condition selection.

Open condition selection, comparison and carbon-equivalent tools for 100CRMO7-4 →

100CrMo7-4 · ISO 683-17-2014

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Bearing steel
Subcategory
Bearing steel
Material form
Reference record
Composition basis
Standard heat-analysis composition
Original record status
Original standard verified
Standard edition
ISO 683-17-2014
Table / clause
Table 3 and footnotes a–k
PDF page references
14、16
Unit
mass fraction (wt%)
Analysis type
Heat analysis; oxygen analysis is separately subject to the manufacturer’s choice

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Default heat-analysis composition in the original table; Manufacturer option: oxygen in heat analysis ≤0.0015%
Applicability of the three welding carbon-equivalent formulas has not been confirmed individually for each bearing-steel group. Only composition is shown; no carbon equivalent from standard ranges is automatically provided.
Default heat-analysis composition in the original table; Machinability by agreement: S≤0.030%; Manufacturer option: oxygen in heat analysis ≤0.0015%
Applicability of the three welding carbon-equivalent formulas has not been confirmed individually for each bearing-steel group. Only composition is shown; no carbon equivalent from standard ranges is automatically provided.
Default heat-analysis composition in the original table; Manufacturer option: oxygen in product analysis ≤0.0015%; not for judging heat-analysis oxygen
Applicability of the three welding carbon-equivalent formulas has not been confirmed individually for each bearing-steel group. Only composition is shown; no carbon equivalent from standard ranges is automatically provided.
Default heat-analysis composition in the original table; Machinability by agreement: S≤0.030%; Manufacturer option: oxygen in product analysis ≤0.0015%; not for judging heat-analysis oxygen
Applicability of the three welding carbon-equivalent formulas has not been confirmed individually for each bearing-steel group. Only composition is shown; no carbon equivalent from standard ranges is automatically provided.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.93 ~ 1.05
Si0.15 ~ 0.35
Mn0.6 ~ 0.8
P≤ 0.025 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
Cr1.65 ~ 1.95
Mo0.4 ~ 0.5
Al≤ 0.05 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)

Applicability and limitations

ISO 683-17:2014 Table 3 and footnotes checked against the original; Table 3 specifies heat analysis, mass fraction wt%; unspecified elements are not treated as zero. Product-analysis deviations are addressed separately in Table 4 and do not expand the default heat-analysis limits.

Composition conditions

Conditional requirement

Original condition-branch records

Default heat-analysis composition in the original table; Manufacturer option: oxygen in heat analysis ≤0.0015%

ElementComposition requirement
C0.93 ~ 1.05
Si0.15 ~ 0.35
Mn0.6 ~ 0.8
P≤ 0.025 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
Cr1.65 ~ 1.95
Mo0.4 ~ 0.5
Al≤ 0.05 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
O≤ 0.0015 (lower limit not stated)
Oxygen-analysis conditions
Heat analysis

Default heat-analysis composition in the original table; Machinability by agreement: S≤0.030%; Manufacturer option: oxygen in heat analysis ≤0.0015%

ElementComposition requirement
C0.93 ~ 1.05
Si0.15 ~ 0.35
Mn0.6 ~ 0.8
P≤ 0.025 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr1.65 ~ 1.95
Mo0.4 ~ 0.5
Al≤ 0.05 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
O≤ 0.0015 (lower limit not stated)
Oxygen-analysis conditions
Heat analysis

Default heat-analysis composition in the original table; Manufacturer option: oxygen in product analysis ≤0.0015%; not for judging heat-analysis oxygen

ElementComposition requirement
C0.93 ~ 1.05
Si0.15 ~ 0.35
Mn0.6 ~ 0.8
P≤ 0.025 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
Cr1.65 ~ 1.95
Mo0.4 ~ 0.5
Al≤ 0.05 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Oxygen-analysis conditions
Product analysis
Separate product oxygen-analysis requirement
Element
O
Upper limit
0.0015
Unit
wt%
Analysis type
Product analysis

Default heat-analysis composition in the original table; Machinability by agreement: S≤0.030%; Manufacturer option: oxygen in product analysis ≤0.0015%; not for judging heat-analysis oxygen

ElementComposition requirement
C0.93 ~ 1.05
Si0.15 ~ 0.35
Mn0.6 ~ 0.8
P≤ 0.025 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr1.65 ~ 1.95
Mo0.4 ~ 0.5
Al≤ 0.05 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Oxygen-analysis conditions
Product analysis
Separate product oxygen-analysis requirement
Element
O
Upper limit
0.0015
Unit
wt%
Analysis type
Product analysis

A condition branch must be selected

Yes

Verification notes

This batch was reconciled against the 2015 DIN German original images and 2014 ISO English original images; edition-specific sources were kept separate, and outdated grades, values and footnote scopes were corrected.

100CrMo7-4 · Ovako Product Catalogue CO-117 ENG 24:07 (2024)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Bearing steel
Subcategory
Bearing steel
Material form
Bars, tubes, rings and precomponents
Composition basis
Manufacturer typical/nominal values, not guaranteed ranges
Original record status
Manufacturer source verified
Document edition
CO-117 ENG 24:07 ©Ovako 2024
Document title
Ovako Product Catalogue
PDF page references
42
Unit
Interpreted as mass fraction (%) using other documents from the same manufacturer; the unit is not explicitly stated in this table
Analysis type
Typical composition analysis
Manufacturer
Ovako

Source document

Carbon-equivalent reference

Manufacturer typical single values are composition references only; no range estimate is made. They are neither standard guarantees nor measured heat results; Formula applicability requires review against the intended use and process.

IIW / CEV: manufacturer typical/nominal single values are shown for reference only; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): manufacturer typical/nominal single values are shown for reference only; standard-range carbon equivalent is not calculated
CET: manufacturer typical/nominal single values are shown for reference only; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
CTypical/nominal value 0.95 (not a guaranteed range)
SiTypical/nominal value 0.3 (not a guaranteed range)
MnTypical/nominal value 0.6 (not a guaranteed range)
CrTypical/nominal value 1.7 (not a guaranteed range)
MoTypical/nominal value 0.4 (not a guaranteed range)

Applicability and limitations

Ovako 2024 product catalogue, PDF page 42; manufacturer’s typical analysis, for composition reference only. The original header does not explicitly state units; interpreted using the manufacturer’s mass-fraction % information. Neither standard guaranteed values nor measured heat analysis. Excluded from limit-based reverse search and carbon-equivalent calculation; blanks and element names alone in the other-elements field are not filled with 0. Manufacturer code: 826.

Conditional requirement

Verification notes

All 170 rows of the 2021 original table were visually checked. Values in corresponding 2024 cells are unchanged; recognition differences were reviewed separately. Rows with conflicting values under the same code are excluded; values are not mixed across sections.

Source notes

Increased hardenability with Cr and Mo for medium- and large-sized components (wall thickness 50 mm).

100CrMo7-4 · Ovako Product Catalogue CO-117 ENG 24:07 (2024)

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Alloy steel
Subcategory
Alloy steel
Material form
Bars, tubes, rings and precomponents
Composition basis
Manufacturer typical/nominal values, not guaranteed ranges
Original record status
Manufacturer source verified
Document edition
CO-117 ENG 24:07 ©Ovako 2024
Document title
Ovako Product Catalogue
PDF page references
66
Unit
Interpreted as mass fraction (%) using other documents from the same manufacturer; the unit is not explicitly stated in this table
Analysis type
Typical composition analysis
Manufacturer
Ovako

Source document

Carbon-equivalent reference

Manufacturer typical single values are composition references only; no range estimate is made. They are neither standard guarantees nor measured heat results; Formula applicability requires review against the intended use and process.

IIW / CEV: manufacturer typical/nominal single values are shown for reference only; standard-range carbon equivalent is not calculated
Pcm (Ito–Bessyo): manufacturer typical/nominal single values are shown for reference only; standard-range carbon equivalent is not calculated
CET: manufacturer typical/nominal single values are shown for reference only; standard-range carbon equivalent is not calculated

Composition

ElementComposition requirement
CTypical/nominal value 0.95 (not a guaranteed range)
SiTypical/nominal value 0.3 (not a guaranteed range)
MnTypical/nominal value 0.6 (not a guaranteed range)
CrTypical/nominal value 1.7 (not a guaranteed range)
MoTypical/nominal value 0.4 (not a guaranteed range)

Applicability and limitations

Ovako 2024 product catalogue, PDF page 66; manufacturer’s typical analysis, for composition reference only. The original header does not explicitly state units; interpreted using the manufacturer’s mass-fraction % information. Neither standard guaranteed values nor measured heat analysis. Excluded from limit-based reverse search and carbon-equivalent calculation; blanks and element names alone in the other-elements field are not filled with 0. Manufacturer code: 826.

Conditional requirement

Verification notes

All 170 rows of the 2021 original table were visually checked. Values in corresponding 2024 cells are unchanged; recognition differences were reviewed separately. Rows with conflicting values under the same code are excluded; values are not mixed across sections.

Source notes

Increased hardenability with Cr and Mo for medium- and large-sized components (wall thickness 50 mm), available as BQ

100CrMo7-4 · DIN EN ISO 683-17-2015

Chemical composition source verified; this does not verify every standard clause, actual supply or measured heat results

Material category
Bearing steel
Subcategory
Bearing steel
Material form
Reference record
Composition basis
Standard heat-analysis composition
Original record status
Original standard verified
Standard edition
DIN EN ISO 683-17:2015-02
Table / clause
Table 3 and footnotes a–k
PDF page references
18、19
Unit
mass fraction (wt%)
Analysis type
Heat analysis; oxygen analysis is separately subject to the manufacturer’s choice

Carbon-equivalent reference

Estimates are presented separately for each applicable composition condition. Match the actual ordering conditions; ranges must not be combined.

Default heat-analysis composition in the original table; Manufacturer option: oxygen in heat analysis ≤0.0015%
Applicability of the three welding carbon-equivalent formulas has not been confirmed individually for each bearing-steel group. Only composition is shown; no carbon equivalent from standard ranges is automatically provided.
Default heat-analysis composition in the original table; Machinability by agreement: S≤0.030%; Manufacturer option: oxygen in heat analysis ≤0.0015%
Applicability of the three welding carbon-equivalent formulas has not been confirmed individually for each bearing-steel group. Only composition is shown; no carbon equivalent from standard ranges is automatically provided.
Default heat-analysis composition in the original table; Manufacturer option: oxygen in product analysis ≤0.0015%; not for judging heat-analysis oxygen
Applicability of the three welding carbon-equivalent formulas has not been confirmed individually for each bearing-steel group. Only composition is shown; no carbon equivalent from standard ranges is automatically provided.
Default heat-analysis composition in the original table; Machinability by agreement: S≤0.030%; Manufacturer option: oxygen in product analysis ≤0.0015%; not for judging heat-analysis oxygen
Applicability of the three welding carbon-equivalent formulas has not been confirmed individually for each bearing-steel group. Only composition is shown; no carbon equivalent from standard ranges is automatically provided.

Composition record (conditional branches apply; this is not an unconditional requirement)

ElementComposition requirement
C0.93 ~ 1.05
Si0.15 ~ 0.35
Mn0.6 ~ 0.8
P≤ 0.025 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
Cr1.65 ~ 1.95
Mo0.4 ~ 0.5
Al≤ 0.05 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)

Applicability and limitations

DIN EN ISO 683-17:2015-02 Table 3 and footnotes checked against the original; the original Table 3 specifies heat analysis, mass fraction wt%; unspecified elements are not treated as zero. Product-analysis deviations are addressed separately in Table 4 and do not expand the default heat-analysis limits.

Composition conditions

Conditional requirement

Original condition-branch records

Default heat-analysis composition in the original table; Manufacturer option: oxygen in heat analysis ≤0.0015%

ElementComposition requirement
C0.93 ~ 1.05
Si0.15 ~ 0.35
Mn0.6 ~ 0.8
P≤ 0.025 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
Cr1.65 ~ 1.95
Mo0.4 ~ 0.5
Al≤ 0.05 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
O≤ 0.0015 (lower limit not stated)
Oxygen-analysis conditions
Heat analysis

Default heat-analysis composition in the original table; Machinability by agreement: S≤0.030%; Manufacturer option: oxygen in heat analysis ≤0.0015%

ElementComposition requirement
C0.93 ~ 1.05
Si0.15 ~ 0.35
Mn0.6 ~ 0.8
P≤ 0.025 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr1.65 ~ 1.95
Mo0.4 ~ 0.5
Al≤ 0.05 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
O≤ 0.0015 (lower limit not stated)
Oxygen-analysis conditions
Heat analysis

Default heat-analysis composition in the original table; Manufacturer option: oxygen in product analysis ≤0.0015%; not for judging heat-analysis oxygen

ElementComposition requirement
C0.93 ~ 1.05
Si0.15 ~ 0.35
Mn0.6 ~ 0.8
P≤ 0.025 (lower limit not stated)
S≤ 0.015 (lower limit not stated)
Cr1.65 ~ 1.95
Mo0.4 ~ 0.5
Al≤ 0.05 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Oxygen-analysis conditions
Product analysis
Separate product oxygen-analysis requirement
Element
O
Upper limit
0.0015
Unit
wt%
Analysis type
Product analysis

Default heat-analysis composition in the original table; Machinability by agreement: S≤0.030%; Manufacturer option: oxygen in product analysis ≤0.0015%; not for judging heat-analysis oxygen

ElementComposition requirement
C0.93 ~ 1.05
Si0.15 ~ 0.35
Mn0.6 ~ 0.8
P≤ 0.025 (lower limit not stated)
S≤ 0.03 (lower limit not stated)
Cr1.65 ~ 1.95
Mo0.4 ~ 0.5
Al≤ 0.05 (lower limit not stated)
Cu≤ 0.3 (lower limit not stated)
Oxygen-analysis conditions
Product analysis
Separate product oxygen-analysis requirement
Element
O
Upper limit
0.0015
Unit
wt%
Analysis type
Product analysis

A condition branch must be selected

Yes

Verification notes

This batch was reconciled against the 2015 DIN German original images and 2014 ISO English original images; edition-specific sources were kept separate, and outdated grades, values and footnote scopes were corrected.