MATERIAL DATA · COLD FORMING

20NiCrMoS6-4 冷镦钢丝

20NiCrMoS6-4 冷镦钢丝技术资料,执行标准为 ISO 4954。查看当前牌号的化学成分、力学性能及相关技术要求。

供货与技术评审 · 睿雄集团受理本产品的供货与技术评审需求;规格、交货状态、数量和检验文件经评审后按订单技术协议确认。

20NiCrMoS6-4 冷镦钢丝 产品图片
20NiCrMoS6-4 · 冷镦钢丝
01执行标准ISO 4954
02材料牌号20NiCrMoS6-4
03材料形态冷镦钢丝
04交货说明按订单技术条件确认

材料技术参数

1.交货条件的组合

表B.1-交货时热处理条件、产品形式和适用要求的组合

原文表头对照:Heat-treatment condition at delivery=交货热处理状态;Symbol=符号;Wire rod=盘条;Bar=棒材;Wire=钢丝。原标准表格、符号及适用条件保留如下。

Heat-treatment condition at deliverySymbolProducts form aApplicable requirements in cases where the steel concerned has been ordered with reference to the steel names indicated in
Wire rodBarWireT a b les B. 2,B.3,B.4 or B.5Ta bles B. 2,B.3,B.4,B.5,B.6 or B,7Optional
As hot-rolled or peeled+AR or +PEXXXChemical composition as specified in Table B.2Mechanical properties as specified in Ta b le s B.3 ,B.4 and B.5Chemical compositior as specified in Table B.2Mechanical properties as specified in Tables B,3, B.4 and B.5Values for hardenability according to Ta ble s B.6 and B.7Supplementa- ry or special requirements as specified in Annex Eh
Cold drawn+AR+C-XX
Cold drawn + spheroidized+AR+C+AC-XX
Cold drawn + spheroidized+skin passed+AR+C+AC +LC-XX
Spheroidized or spheroidized+peeled+AC or +AC +PEXXX
Spheroidized+cold drawn+AC+CXX
Treated to ferrite- pearlite structure and hardness range+FP-X-
OthersOther delivery conditions may be agreed at the time of ordering
a X=applicable,-=not applicable. b If agreed at the time of the enquiry and order.

2.化学组成

表B.2-表面硬化用钢的化学成分 (适用于熔炼分析)

表B.2-表面硬化用钢的化学成分 (适用于熔炼分析)

Steel name b% mass fraction a
CSi cMnPSCrNiMoBCu
20NiCrMoS6-40,16 to 0,230,300,50 to 0,900,0250,020 to 0,0400,60 to 0,901,40 to 1,700,25 to 0,35—0,25
Elements not quoted in this table should not be intentionally added to the steel without the agreement of the purchaser,except those intended for finishing the heat.All reasonable precautions shall be taken in order to prevent the addition of such elements from scrap or other materials used in the production process,which can affect the hardenability, mechanical properties and applicability To improve the performance of cold heading,it is possible to add Al:0,020 %to 0,050 % a Maximum values unless otherwise indicated. b In the case of steels with hardenability requirements (see Ta bles B. 6 and B.7),minor deviations from the specified limits are permitted (with the exception of sulfur and phosphorus),provided that they do not exceed 0,01 %for carbon and the values indicated in Table 2 for the other elements. c A lower silicon content or a specific silicon range may be agreed at the time of ordering.

3.力学性能

表B.5-合金钢牌号的力学性能

表B.5-合金钢牌号的力学性能 (续)

Steel nameDiameterDelivery condition
+AC+FP+AR+C+AC+AR+C+AC+LC+AC+C
above mmup to mmRm max. MPaZ min %HB Min.max.Rm max. MPaZ min %Rm max. MPaZ min. %Rm max. MPaZ min. %
20NiCrMoS6-4256106065058—
51061058149201590606305873055
102561058149201590606305872055

4.淬透性要求

表B.6-标准淬透性钢种的硬度限值 (H级)

表B.6-标准淬透性钢种 (H级) 的硬度限值 (续)

Steel nameSymbolAustenitizing temperature °℃±5℃Limits of rangeHardness HRC at a distance from quenched end of test piece(in mm)of
1,535791113152025303540
20NiCrMoS6-4+H880max.49494848474746444139383736
min.41403936333028262321———

表B.7-具有限制淬透性散射带的钢种的硬度限值 (HH和HL等级)

表B.7-淬透性受限的钢种分散带 (HH和HL等级) 的硬度限值 (续)

Steel nameSymbolAustenitizing temperature ℃±5℃Limits of rangeHardness HRC at a distance from quenched end of test piece(in mm)of
1,535791113152025303540
20NiCrMoS6-4+HH880max49494848474746444139383736
min.44434240383634322927262524
+HLmax46464544424140383533323130
min.41403936333028262321——

使用与订购说明

化学成分、力学性能、交货状态及其他技术要求应以现行有效标准、客户图纸和订单技术协议为准;网页资料不替代正式质量证明文件。

询盘建议提供资料

碳当量计算器 — 20NiCrMoS6-4

依据: ISO 4954

化学成分依据: ISO 4954:2018

按所列标准原文转录

来源原文

Table B.2

IIW / CEV

CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15已知项贡献,非完整值: 0.5067–0.7600

缺少元素: V

IIW/CEV:碳钢和低合金钢的焊接性初筛。

Pcm (Ito–Bessyo)

Pcm = C + Si/30 + (Mn + Cu + Cr)/20 + Ni/60 + Mo/15 + V/10 + 5B已知项贡献,非完整值: 0.2550–0.3942

缺少元素: V, B

Pcm:主要适用于低碳低合金钢;尤其 C 超过 0.11% 时,须另行确认适用性。

CET

CET = C + (Mn + Mo)/10 + (Cr + Cu)/20 + Ni/40计算范围: 0.3000–0.4550

CET:铁素体钢焊接预热评估,须核对 EN 1011-2 的适用条件。

单侧上限表示从 0 到该上限;只有下限时不能确定上界。缺项未知,不按零处理。标准极限组合值不是炉批实测值。

碳当量辅助评估焊接性,不代表冷镦、紧固件强度或焊接工艺获准。上述公式不直接适用于不锈钢、铸铁及有色金属。